您现在位置:兽药智库> 处方工艺> BASF处方集> 浏览文章
ProtectiveFilmCoatingwithKollidonVA64
HydroxypropylCellulose
1.Formulations
No.1No.2
(Subcoating(Final
coating)
KollidonVA64[1]...........................................20g20g KlucelEF(Hercules).....................................20g20g Talc....................................................................–20g SicovitIronoxide[1].......................................q.s.q.s.
Isopropanol..................................................760g–
Water.................................................................–740g 2.Manufacturingofthesuspension
DissolveKlucelandKollidonVA64inisopropanolorwaterandsuspend
thecolorantsandthetalc.Passthismixturethroughacolloidmill.
3.Coatingprocedure(Sugarcoatingpan)
No.1No.2
Loadingoftabletcores
(9mm,biconvex,surface3cm2).....................2kg2kg Amounto fcoatingsuspension..................<800g800g Sprayphase.....................................................6s3s
Interval..........................................................0.5s0.5s
Dryingphase(warmair)....................................6s6s
Interval............................................................2s2s
Nozzle(WaltherWAXV).............................0.8mm0.8mm
Quantityofsprayedsuspension/min..............25g6.8g Quantityofsolidsappliedoneach
tabletcore<3.2mg.......................................<1h3.1mg to talcoatingtime...........................................<1h5–6h